Add an emulsifier equivalent to 3% of the total monomer amount to the polymerization kettle, add deionized water, stir and dissolve, raise the temperature to 60 ℃, add 0.4% ammonium persulfate as the initiator, and then add 30% of the mixed monomers. When the temperature rises to around 80 ℃, slowly add the remaining two-thirds of the monomers. After adding the monomers, raise the temperature to 95 ℃~98 ℃ and stir for 0.5h, cool, and adjust the pH value with water. Finished product.